Description:
Ceramic magnet material (Ferrite) is one of the most cost effective magnetic materials, it has a fair to good resistance toward corrosion and it can operate in moderate heat. Ceramic (Ferrite) magnets have low energy product and they are usually used in assemblies containing mild steel.
Production Process Flowchart:
Magnetic Properties:
Mat. | Br | bHc | iHc | BHmax | ||||
mT | KG | KA/m | KOe | KA/m | KOe | KJ/m³ | MGOe | |
Y10T | 200~235 | 2.0~2.35 | 125~160 | 1.57~2.01 | 210~280 | 2.64~3.52 | 6.5~9.5 | 0.8~1.2 |
Y20 | 320~380 | 3.2~3.8 | 135~190 | 1.70~2.38 | 140~195 | 1.76~2.45 | 18.0~22.0 | 2.3~2.8 |
Y22H | 310~360 | 3.1~3.6 | 220~250 | 2.77~3.14 | 280~320 | 3.52~4.02 | 20.0~24.0 | 2.5~3.0 |
Y23 | 320~370 | 3.2~3.7 | 170~190 | 2.14~2.38 | 190~230 | 2.39~2.89 | 20.0~25.5 | 2.5~3.2 |
Y25 | 360~400 | 3.6~4.0 | 135~170 | 1.70~2.14 | 140~200 | 1.76~2.51 | 22.5~28.0 | 2.8~3.5 |
Y26H | 360~390 | 3.6~3.9 | 220~250 | 2.77~3.14 | 225~255 | 2.83~3.21 | 23.0~28.0 | 2.9~3.5 |
Y27H | 370~400 | 3.7~4.0 | 205~250 | 2.58~3.14 | 210~255 | 2.64~3.21 | 25.0~29.0 | 3.1~3.7 |
Y30 | 370~400 | 3.7~4.0 | 175~210 | 2.20~2.64 | 180~220 | 2.26~2.77 | 26.0~30.0 | 3.3~3.8 |
Y30BH | 380~390 | 3.8~3.90 | 223~235 | 2.80~2.95 | 231~245 | 2.90~3.08 | 27.0~30.0 | 3.4~3.7 |
Y30-1 | 380~400 | 3.8~4.0 | 230~275 | 2.89~3.46 | 235~290 | 2.95~3.65 | 27.0~32.0 | 3.4~4.0 |
Y30-2 | 395~415 | 3.95~4.15 | 275~300 | 3.46~3.77 | 310~335 | 3.90~4.21 | 28.5~32.5 | 3.5~4.0 |
Y32 | 400~420 | 4.0~4.2 | 160~190 | 2.01~2.38 | 165~195 | 2.07~2.45 | 30.0~33.5 | 3.8~4.2 |
Y33 | 410~430 | 4.1~4.3 | 220~250 | 2.77~3.14 | 225~255 | 2.83~3.21 | 31.5~35.0 | 4.0~4.4 |
Y35 | 400~410 | 4.00~4.10 | 175~195 | 2.20~2.45 | 180~200 | 2.26~2.51 | 30.0~32.0 | 3.8~4.0 |
Typical Physical Properties:
Curie Temperature (°C) | 450 |
Maximum Operating Temperature (°C) | 250 |
Hardness (Hv) | 480-580 |
Density (g/cm3) | 4.8 – 4.9 |
Relative Recoil Permeability (µrec) | 1.05 – 1.20 |
Saturation Field Strength, kOe (kA/m) | 10 (800) |
Temperature Coefficient of Br (%/°C) | -0.2 |
Temperature Coefficient of iHc (%/°C) | 0.3 |
Tensile Strength (N/mm) | <100 |
Transverse Rupture Strength (N/mm) | 300 |